Phenomenon description

The film is peeled off or rolled up from a large area on the wall, usually revealing the substrate.


Cause Analysis

1. The moisture content of the substrate exceeds the standard and affects the adhesion of the paint layer.

2. The base or putty is loose and the strength is not enough. The paint layer only adheres to the surface of the powder layer.

3. The ambient humidity during construction is too high and there is condensation on the surface of the substrate.

4. The substrate has grease or mold release agent residue, affecting paint adhesion.

5. The substrate has no roughness, the mechanical bite and force of the paint layer is not enough.


Solution

1. After the eradication, the layer is treated, and the base layer is recoated after meeting the requirements.

2. The construction conditions must be guaranteed during construction, and the ambient humidity is less than 85%.

3. The substrate must be clean and free of grease. It can be cleaned with a solvent.

4. The flatness of the surface of the putty layer should meet the requirements and should maintain a certain roughness.

Home· BaoJun· Construction Coating· Industrial Coating· Solution· Project· Service· Intelligent Manufacturing

Address:No. 9 Chuangxin Avenue, Binhai Science and Technology Park, Binhai High-tech Zone, Tianjin,China Zip code:300457

National Hotline

400-022-5055

Copyright © 2019 BaoJunPaint.com All Rights Reserved. 版权所有 宝骏涂料 京ICP备12053088号-1